GH4105是(shi)Ni-Co-Ci-基(ji)積淀硬底化(hua)型(xing)形變中高(gao)溫(wen)不銹鋼,動用(yong)的溫(wen)度(du)(du)750℃-950℃。鋁合金的在常溫(wen)和(he)溫(wen)度(du)(du)過高(gao)強度(du)(du)較(jiao)高(gao),化(hua)性(xing)(xing),但熱代(dai)加(jia)工性(xing)(xing)和(he)激光焊接(jie)性(xing)(xing)基(ji)本上(shang)。使(shi)應用(yong)于(yu)生產加(jia)工航材(cai)(cai)起行(xing)為增壓樹葉、溫(wen)度(du)(du)過高(gao)螺(luo)栓標準等溫(wen)度(du)(du)過高(gao)零(ling)機件(jian)。核心(xin)產品設備有熱軋鋼棒(bang)材(cai)(cai)和(he)扁材(cai)(cai)、冷拉棒(bang)材(cai)(cai)、塑鋼型(xing)材(cai)(cai)和(he)環型(xing)件(jian)等。
GH4105化學上(shang)的(de)材(cai)料
事物 | C | Cr | Ni | Co | Mo | Al | Ti | Fe | B |
質量分數(shu)/% | 0.12-0.17 | 14.0-15.7 | 余 | 18.0-22.0 | 4.5-5.5 | 4.5-4.9 | 1.18-1.5 | ≤1.0 | 0.003-0.010 |
物質 | Mn | Si | P | S | Cu | Ag | Bi | Pb | Zr |
質(zhi)量分數/% | ≤0.40 | ≤0.25 | ≤0.015 | ≤0.01 | ≤0.200 | ≤0.0005 | ≤0.0001 | ≤0.0010 | 0.07-0.15 |
GH4105運動學及運動學性(xing)
體積密度 | 沸點 |
7.97g/cm3 | 1340-1380℃ |
款式 | 熱工作 | σb/MPa | σp0.2/MPa | δ5/% |
螺帽用冷拉棒 | 規則熱外理 | ≥1000 | ≥680 | ≥18 |
GH4105熱操作系統(tong)
茶(cha)葉(xie)用軋鋼棒和扁 材、鍛件,1150℃±10℃*4h/AC+1030℃±10℃*16h/AC+ 700℃±5℃*16h/AC;
冷拉棒(bang),1125℃±10℃/AC+850℃±10℃*16h/AC,其中的固溶(rong)隔(ge)熱時期(qi):d≤3mm,1h;d>3mm-6mm,2h;d>6mm-40mm,4h。
GH4105數據由滬隆(long)繼(ji)輕金屬(shu)投資控股公司(si)全程(cheng)提供,你(ni)可搜索(suo)更(geng)多(duo)了解(jie)重(zhong)慶隆(long)繼(ji)廢金屬(shu)國(guo)際(ji)公司(si)。